dc.creator.ID |
PATRICIO, S. M. R. |
pt_BR |
dc.creator.Lattes |
http://lattes.cnpq.br/9872880548902941 |
pt_BR |
dc.contributor.advisor1 |
NEVES, Gelmires de Araújo. |
|
dc.contributor.advisor1ID |
NEVES, G. A. |
pt_BR |
dc.contributor.advisor1Lattes |
http://lattes.cnpq.br/3167458244674160 |
pt_BR |
dc.contributor.advisor2 |
CARVALHO, João Batista Queiroz de. |
|
dc.contributor.advisor2ID |
CARVALHO, J. B. Q. |
|
dc.contributor.advisor2Lattes |
http://lattes.cnpq.br/1833502684638113 |
|
dc.contributor.referee1 |
FERREIRA, Heber Carlos. |
|
dc.contributor.referee2 |
OLIVEIRA, Djane de Fátima. |
|
dc.description.resumo |
No Brasil existem sérios problemas ambientais no que se refere a extração
indiscriminada de recursos naturais e a constante geração de resíduos de
construção e demolição. Buscando soluções que minimizem esta degradação
ambiental, procuramos desenvolver novas técnicas de reutilização e reciclagem dos
resíduos da construção civil para fabricação de materiais alternativos, incentivando o
desenvolvimento sustentável. Com o objetivo de se obter aglomerante pozolânico a
partir da reciclagem de resíduos da construção civil, oriundos de demolição visando
sua aplicação na fabricação de tijolos solo-cal. Foram realizados estudos em uma
amostra de resíduo de demolição, proveniente da reforma do laboratório de Solos I,
um solo proveniente de jazida e uma amostra de cal. As amostras foram submetidas
a ensaios de caracterização física, química e mineralógica, como: granulometria,
limites de liquidez e plasticidade, massa especifica real, analise química, analise
térmica diferencial, difração de raios-X, área especifica e determinação da atividade
pozolânica. O resíduo de demolição foi triturado em moinho de galga, ate a obtenção
de uma distribuição granulométrica próxima da cal. Foram moldados corpos de
prova de solo-cal no trago 1:10 em peso, e solo-cal com incorporação de resíduos
nas seguintes proporções: 0%, 10%, 20%, 30%, 40%, 50% e 75%. Posteriormente
foram confeccionados tijolos de solo-cal e solo-cal-resíduo com 25% de resíduo,
uma vez que estudos com os corpos de prova, com esta composição, apresentaram
melhores resultados. Os corpos de prova e os tijolos foram curados por períodos de
28, 60 e 90 dias de cura e submetidos a ensaios de resistência a compressão
simples e absorção, cujos resultados apresentaram comportamento mecânico dentro
das normas da ABNT e que existe viabilidade técnica no aproveitamento de resíduo
de demolição para uso na fabricação de tijolos solo-cal incorporados com resíduo
sem função estrutural e que seu uso implica na preservação do meio ambiente e na
melhoria da qualidade de vida da população em geral. |
pt_BR |
dc.publisher.country |
Brasil |
pt_BR |
dc.publisher.department |
Centro de Tecnologia e Recursos Naturais - CTRN |
pt_BR |
dc.publisher.program |
PÓS-GRADUAÇÃO EM ENGENHARIA CIVIL E AMBIENTAL |
pt_BR |
dc.publisher.initials |
UFCG |
pt_BR |
dc.title |
Aproveitamento de resíduos da construção civil na produção de tijolos solo-cal. |
pt_BR |
dc.date.issued |
2011-05 |
|
dc.description.abstract |
In Brazil there are serious environment problems regarding the indiscriminate
extraction of natural resources and constant generation of construction and
demolition waste. Researching solutions to minimize this degradation, new
techniques for reusing and recycling of construction waste for the production of
alternative materials have been developed, encouraging sustainable development.
With the aim of obtaining pozzolonic binder from recycling of construction waste, for
its application in the manufacture of soil-lime bricks, it was studied a sample of
demolition waste, from the reform of Soil Laboratory I, a soil and a sample of lime.
The samples were characterized by chemical analysis, thermogravimetric analysis,
X-ray diffraction, surface area and determination of pozzolanic activity. The
demolition waste was milled in mill climbs, until obtaining a particle size similar to the
lime. Specimens were prepared for test-soil-lime and lime-soil-residue on the das and
1:10, as binders and lime waste from demolition, the following compositions: 0%,
10%, 20%, 30%, 40%, 50% and 75% waste and soil as aggregate. Then, they were
made of soil-lime bricks incorporated with 25% waste, what is the best composition of
the specimens used in evidence. The specimens and the bricks were cured for
periods of 28, 60 and 90 days and tested for determine unconfined compressive
strength and absorption, which showed that the recycling of waste demolition
presented itself as a promising material to be used in the manufacture of bricks used
in buildings and that its use implies the preservation of the environment and
improving the quality of population lives in general. But it's necessary further study in
relation to standardization. The results were not satisfactory with the demolition
waste as a binder. |
pt_BR |
dc.identifier.uri |
http://dspace.sti.ufcg.edu.br:8080/jspui/handle/riufcg/11849 |
|
dc.date.accessioned |
2020-02-13T10:11:38Z |
|
dc.date.available |
2020-02-13 |
|
dc.date.available |
2020-02-13T10:11:38Z |
|
dc.type |
Dissertação |
pt_BR |
dc.subject |
Resíduos de Demolição |
|
dc.subject |
Tijolos |
|
dc.subject |
Solo-cal |
|
dc.subject |
Pozolana |
|
dc.subject |
Aproveitamento de Resíduos |
|
dc.subject |
Construção Civil |
|
dc.subject |
Demolition Waste |
|
dc.subject |
Bricks |
|
dc.subject |
Soil-lime |
|
dc.subject |
Pozzolana |
|
dc.subject |
Use of Waste |
|
dc.subject |
Buildings |
|
dc.rights |
Acesso Aberto |
pt_BR |
dc.creator |
PATRICIO, Solange Maria da Rocha. |
|
dc.publisher |
Universidade Federal de Campina Grande |
pt_BR |
dc.language |
por |
pt_BR |
dc.title.alternative |
Use of construction waste in the production of soil-lime bricks. |
pt_BR |
dc.identifier.citation |
PATRICIO, Solange Maria da Rocha. Aproveitamento de resíduos da construção civil na produção de tijolos solo-cal. 2011. 91f. (Dissertação de Mestrado em Engenharia Civil e Ambiental), Programa de Pós-Graduação em Engenharia Civil e Ambiental, Universidade Federal de Campina Grande - Paraíba - Brasil, 2011. Disponível em: http://dspace.sti.ufcg.edu.br:8080/jspui/handle/riufcg/11849 |
pt_BR |